Case Studies of Fatigue Life Improvement Using Low Plasticity Burnishing in Gas Turbine Engine Applications

Paul S. Prevéy, Ravi A. Ravindranath, Michael Shepard, Timothy Gabb

Abstract

Surface enhancement technologies such as shot peening, laser shock peening, and low plasticity burnishing (LPB) can provide substantial fatigue life improvement. However, to be effective, the compressive residual stresses that increase fatigue strength must be retained in service. For successful integration into turbine design, the process must be affordable and compatible with the manufacturing environment. LPB provides thermally stable compression of comparable magnitude and even greater depth than other methods, and can be performed in conventional machine shop environments on CNC machine tools. LPB provides a means to extend the fatigue lives of both new and legacy aircraft engines and ground-based turbines. Improving fatigue performance by introducing deep stable layers of compressive residual stress avoids the generally cost prohibitive alternative of modifying either material or design. The x-ray diffraction based background studies of thermal and mechanical stability of surface enhancement techniques are briefly reviewed, demonstrating the importance of minimizing cold work. The LPB process, tooling, and control systems are described. An overview of current research programs conducted for engine OEMs and the military to apply LPB to a variety of engine and aging aircraft components are presented. Fatigue performance and residual stress data developed to date for several case studies are presented including the following. (1) The effect of LPB on the fatigue performance of the nickel based super alloy IN718, showing the fatigue benefit of thermal stability at engine temperatures. (2) An order of magnitude improvement in damage tolerance of LPB processed Ti-6-4 fan blade leading edges. (3) Elimination of the fretting fatigue debit for Ti-6-4 with prior LPB. (4) Corrosion fatigue mitigation with LPB in Carpenter 450 steel. (5) Damage tolerance improvement in 17-4 PH steel. Where appropriate, the performance of LPB is compared to conventional shot peening after exposure to engine operating temperatures. [DOI: 10.1115/1.1807414]

Introduction

LPB is a new method of surface enhancement [1–4] that provides deep stable surface compressive residual stresses with little cold work for improved fatigue, fretting fatigue, and stress corrosion performance even at elevated temperatures where compression from shot peening relaxes [5]. LPB surface treatment is applied using conventional multi-axis CNC machine tools for unprecedented control of the residual stress distribution developed through modification of the pressure, feed, and tool characteristics. The resulting deep layer of compressive residual stress has been shown to improve high cycle fatigue (HCF) and low cycle fatigue (LCF) performance and foreign object damage (FOD) tolerance [6,7]. Achieving deep compression with low cold work (<5%) reduces relaxation of the protective compressive layer either thermally during exposures at service temperatures, or mechanically due to overload or impact, as in FOD. Both thermal and mechanical relaxation occur in the cold worked surfaces produced by conventional shot peening of titanium [7] and nickel alloys [5,6].

The LPB tooling and process are described and the protocol for use of LPB in fatigue-critical design is presented. LPB has been applied to titanium, iron, and nickel based aero-turbine engine alloys to improve damage tolerance in compressor sections by an order of magnitude and to improve high and low cycle fatigue performance in hot turbine sections. In addition to turbine engine components, this novel technology has been shown to have potential applications in aging aircraft structures, nuclear waste-material containers, biomedical implants and welded joints. This paper attempts to present a brief overview of the fatigue and damage tolerance improvement achievable with LPB in aero engine components.

The Low Plasticity Burnishing (LPB) Process

LPB is a method of CNC controlled burnishing designed to produce a deep layer of highly compressive residual stress with a minimum amount of cold working, or plastic deformation. Residual compressive stresses approaching the material yield strength are developed using a series of passes of a freely rotating ball tool producing an accumulated plastic strain, or cold work, level of less than 3% to 5%. In contrast, the multiple random shot impacts of conventional shot peening produce cold work levels ranging from 20% to over 100%, leaving a severely deformed surface layer with a high dislocation density that adversely affects the thermal and mechanical stability of the compressive layer [5,7].

Unlike LPB, conventional roller and ball burnishing utilize a hard wheel tool or fixed lubricated ball pressed into the surface of an axisymmetric work piece with sufficient force to deform the near surface layers, usually in a lathe. Burnishing is performed with multiple passes, usually under increasing load, to improve surface finish and to deliberately cold work the surface. Roller and ball burnishing have been studied in Russia and Japan, and were applied most extensively in the USSR in the 1970s. Various burnishing methods are used, particularly in Eastern Europe to im- [text continues beyond the screenshot]

Fig. 1 LPB schematic

 

prove fatigue life. Improvements in HCF, corrosion-fatigue, and stress corrosion cracking are documented, with fatigue strength enhancement attributed to improved finish, the development of a compressive surface layer, and the increased yield strength of the cold worked surface 8–13-. Optimum forces and rolling parameters were established to minimize roughness and/or maximize surface hardening 14–17-. Analytical models to predict the residual stresses have been attempted in England 18 and France 19-. ”Deep rolling” employs either roller tools or a partially hydrostatically supported burnishing ball, but differs from LPB in the use of higher loads and cold work levels, tool design, and control. X-ray diffraction line broadening and micro-hardness reveal that deep rolling produces even more cold work than shot peening 20–22-.

The basic LPB tool is comprised of a ball that is supported in a spherical hydrostatic bearing as shown in Fig. 1. The tool can be held in any CNC lathe or mill. The machine tool coolant is used to pressurize the bearing with a continuous flow of fluid to support the ball. The ball does not contact the bearing seat, even under load. The ball is loaded normal to the surface of a component with a hydraulic cylinder that is in the body of the tool. LPB can be performed in conjunction with chip forming machining operations in the same CNC machine tool.

The ball rolls across the surface of a component in a pattern defined in the CNC code, as in any machining operation. The tool path and normal pressure applied are designed to create a distribution of compressive residual stress. The form of the distribution is designed to counter applied stresses and optimize fatigue or stress corrosion performance. Since there is no shear being applied to the ball, it is free to roll in any direction. As the ball rolls over the component, the pressure from the ball causes plastic deformation to occur in the surface of the material under the ball. Since the bulk of the material constrains the deformed area, the deformed zone is left in compression after the ball passes. No material is removed during the process. The surface is permanently displaced inward by only a few ten-thousandths of an inch 0.002–0.015 mm0.0001–0.0006 in.. LPB smoothes surface asperities leaving an improved surface finish that can be better than 5 in., RA. Dual sided LPB processing of a 17-4 PH compressor blade with caliper tooling and a larger finished Ti-6-4 blade are shown in Figs. 2a and 2b.

X-ray Diffraction, Residual Stress and Cold Work Determination

XRD residual stress measurements were made employing a sin2 technique and the diffraction of the appropriate radiation. It was first verified that the lattice spacing was a linear function of sin2 as required for the plane stress linear elastic residual stress model 23–26-.

Measurements were made as a function of depth by incremental electropolishing to the final depth shown. The residual stress measurements were corrected for both the penetration of the radiation into the subsurface stress gradient 27 and for stress relaxation caused by layer removal 28-.

The value of the x-ray elastic constants required to calculate the macroscopic residual stress from the crystal lattice strain were determined in accordance with ASTM E1426-91 29-. Systematic errors were monitored per ASTM specification E915.

The K1 peak breadth was calculated from the Pearson VII function fit used for peak location during macroscopic stress measurement 30-. The percent cold work was calculated using an empirical relationship established between the material cold working true plastic strain and the K 1 line broadening 31-. The percent cold work is a scalar quantity, taken to be the true plastic strain necessary to produce the diffraction peak width measured based on the empirical relationship.

Thermal Stability of LPB Residual Stress Distributions

Surface enhancement methods introduce a layer of compression on the surface of a component to enhance HCF performance or to mitigate the fatigue or stress corrosion debit caused by pitting corrosion, FOD, or other surface damage. Historically, shot peening SP has been widely used to significantly improve HCF performance. However, the heavy surface cold work, surface roughness, and potential surface damage associated with SP limit the range of application. The high degree of cold work produced by SP leads to both thermal and mechanical relaxation 5,7-, and may leave the surfaces more prone to corrosion related damage. In contrast, LPB inherently produces little cold work in developing a deep layer high compression. LPB processing parameters including ball size, type, applied pressure/vertical displacement, lateral velocity, feed, work piece mechanical properties, etc., are developed for a given material and geometry using x-ray diffraction measurement of residual stress and cold work distributions. Discussion of the LPB parameter development is beyond the scope of this paper.

Depending on the LPB process parameters and material characteristics, the residual stress state and the corresponding percent cold work both depth profile and surface distribution vary as functions of position. A large database has been developed to document these distributions for a variety of structural engineering materials of interest to aerospace, automotive, nuclear, and biomedical applications. A typical set of residual stress and corresponding percent cold work depth profiles for IN718 are shown in Fig. 3. The effects of thermal exposure to 525 and 600°C on the residual stress profiles are included. For the sake of comparison, typical results from shot peened SP surfaces given the same thermal exposure are included in these figures. Similar thermal relaxation studies have been conducted in many other material systems of interest to the turbine engine industry. Figure 4 shows the relaxation effects in LPB processed Ti-6Al-4V after exposure to 425°C.

In the IN718 example, it is seen that the LPB process achieved compression to a depth exceeding 1 mm 0.04 in., reaching a maximum of nominally -1100 MPa -159.6 ksi at nominally 250 m 0.01 in. with less than 5% cold work through the compressive zone. In contrast, SP produced a depth of compression less than 250 m 0.01 in. with over 60% cold work on the surface. Retention of surface compression is important in HCF where suppression of surface fatigue initiation typically governs life. After 100 hours of exposure to 525°C, the LPB processed material showed very little relaxation of residual stress at the surface, while the SP processed material lost surface compression from over -800 MPa -116 ksi to under -100 MPa 14.5 ksi. This stress relaxation is attributed to the heavy cold work experienced by SP, leading to rapid recovery and stress relaxation during

Fig. 2 „a… 17-4 PH compressor blade being processed on the leading edge „LE… with an LPB caliper tool to improve FOD tolerance; „b… Ti-6-4 fan blade LPB processed along the lower LE. The hole near tip was made for HCF testing in cantilever bending „see Fig. 8…

 

thermal exposure 5-. Similar thermal relaxation data have been obtained for LPB and SP in a number of Ti, Fe and Al alloys and similar response to thermal exposure have been observed 6,7-. Using larger tools and higher pressures, compression up to 8 mm 0.3 in. depth has recently been achieved in stainless steel welded plates.

Fatigue Testing

HCF tests were conducted on specially designed test specimens to simulate the service conditions of the components. For this purpose, thick section 9.5 mm 0.37 in.specimens with trapezoidal cross section designed for testing highly compressive surfaces or a blade-edge feature cross section were tested under a four-point bending load with the capability to vary applied R ratios ( min /max). Crack propagation for the thick section samples was from the surface through the depth of the compressive layer. Blade-edge samples were processed to produce through-thickness compression and tested with the crack propagating from the edge, perpendicular to the processed surfaces. In most instances, an R ratio of 0.1 was used to simulate the high mean load common to rotating turbine components. HCF tests were run at a frequency of 30 Hz to either failure or a run-out condition of 2.5106 cycles.

Engine operating conditions were simulated in several ways. For example, typical FOD conditions were simulated by either pressing an indentation, machining a notch, or using electrodischarge machining EDM. To simulate exposure to engine temperatures, specimens were typically exposed to engine operating temperatures for a fixed time before HCF testing to allow thermal relaxation. Active corrosion was simulated by wrapping pads soaked in corroding media around the samples for the duration of the test. Fretting fatigue was simulated using a specially designed ”bridge” fretting fixture with variable fretting normal loads Fig. 13.

Effect of LPB on HCF Performance and FOD Tolerance

The thick section HCF results for IN718 presented in Fig. 5 show a substantial increase in the HCF endurance limit, or fatigue strength at 2106 cycles for LPB over shot peening for either 525 or 600°C exposure for 100 h. The similar fatigue performance for shot peening followed by either 525 or 600°C exposure is attributed to the near uniform relaxation of the surface compression seen in Fig. 3 after exposure to either temperature. The endurance limit is typically associated with surface residual compression governing the initiation of fatigue cracks while fatigue strength in the finite life regime is dominated by crack growth through the depth of the compressive layer left by surface enhancement.

Fig. 3 Residual stress and cold work depth profiles for IN718 before and after exposure to service temperature of 525 and 600°C for 100 h

 

The difference in the ability of the two surface enhancement methods to resist FOD either in the form of a single indentation or a sharp notch is shown in Fig. 6. The endurance limit is reduced from nominally 700 to 300 MPa 101. to 43.5 ksi by either form of damage. The deep compressive layer produced by LPB is more effective in retarding crack growth, even after thermal exposure, because of the minimal thermal stress relaxation and the greater depth of the compressive layer. Although considerable scatter is

Fig. 4 Thermal relaxation of shot peened „8 A, 400%… and LPB processed Ti-6Al-4V after 795°F „425°C… for 10 h

Fig. 5 High cycle fatigue performance of shot peened ” 8 A, 400% … and LPB processed thick section IN718 after 100 h, exposures at 525 and 600°C

 

evident in the LPBFOD data which is attributed to variability in the FOD damage all of the specimens treated by LPB have fatigue strengths and lives superior to that of shot peening even without FOD.

HCF data for thick section Ti-6Al-4V shows similar trends in Fig. 7. The HCF results presented in this figure show a 38% increase in the endurance limit for LPB 620 MPa 90 ksicompared to shot peening 448 MPa 65 ksi after exposure to 425°C 795°F for 10 h. The increased endurance limit after surface enhancement is generally associated with surface compression delaying the initiation of fatigue cracks at the surface. The reduced HCF strength of the highly cold worked shot peened condition is attributed to the complete loss of surface compression after even a brief elevated temperature exposure.

Improved Damage Tolerance in Aero Engine Components

LSP of the leading edges of fan and compressor blades improves damage tolerance, in terms of FOD depth, by at least an oder of magnitude. The high magnitude through-thickness compression achieved by LSP retards both fatigue crack initiation and growth, but requires expensive specialized laser systems. LPB has been

Fig. 6 HCF tolerance of dull and sharp FOD after elevated temperature exposure simulating engine environments for shot peened ” 8 A, 400% … and low plasticity burnished ” LPB … thick section IN 718

Fig. 7 HCF performance of thick section Ti-6-4 after SP and LPB surface treatments with and without the presence of a 250 m ” 0.01 in. … FOD after exposure to service temperatures

 

investigated as a means of inducing through-thickness leading edge compression for improved damage tolerance in first stage Ti-6-4 fan blades. Fatigue performace was assessed by testing actual fan blades with controlled depth simulated leading edge FOD.

To establish the appropriate depth of simulated FOD, size and location distributions of service generated FOD were documented for used blades. Service induced FOD on the leading edge ranged from 0.005 mm 0.0002 in. to less than 0.50 mm 0.02 in. deep. Ninety percent of FOD depths observed were less than 0.05 mm 0.002 in.. Blades are currently removed for re-work or replacement if FOD 0.13 mm 0.005 in. deep is found durning inspection. Conservatively, 0.50 mm was chosen as the minimum depth for FOD to be induced in blades for this study. Simulated FOD 0.5 mm 0.02 in. and 1.2 mm 0.05 in. in depth was created by machining 60° ”V” notches in blades in the leading edge location at which maximum stress occurred during fatigue loading.

LPB processing CNC code was designed and LPB parameters developed to create through-thickness compression of nominally -689 MPa -100 ksi from the blade leading edge to a nominal distance of 6.4 mm 0.25 in. chord-wise from the leading edge. The extent of the LPB zone running along the leading edge, from the midspan damper to the platform, may be seen clearly as the region of improved surface finish in Fig. 2b.

Fatigue comparisons were made using used blades as test specimens cantilever loaded at R 0.1 to simulate the high mean load imposed on the leading edge during service in a rotating engine, as shown in Fig. 8. The S-N curves developed are shown in Fig. 9. In the absence of FOD, LPB processing increased fatigue strength by nominally 207 MPa 30 ksi over nonprocessed blades, and approached the material yield strength. In all but one instance, LPB processed blades tested without FOD at such high stress levels failed outside the most highly stressed LPB-processed area, usually in the dovetail region.

Introduction of 0.5 mm 0.02 in. deep simulated FOD in non-LPB blades reduced the fatigue strength 65% from 689 to 241 MPa 100 to 35 ksi. Introduction of the same 0.5 mm 0.02 in FOD after LPB processing resulted in fatigue strength equal to that of non-LPB processed blades without FOD. FOD 1.27 mm 0.05 in. deep after LPB reduced the fatigue strength to 620 MPa 90 ksi, only 10% less than the strength of unprocessed blades. Similarly, Fig. 10 shows the beneficial effects of LPB in mitigating HCF damage and improving FOD tolerance in a Ti-6-4 low

Fig. 8 Photograph showing the cantilever-loading fixture for fatigue testing of the first stage fan blade. Note the LPB patch along the ” upper … leading edge of the blade.

Fig. 9 Effect of LPB in mitigating HCF and FOD damage in Ti-6-4 fan blades

 

pressure vane LPB processed to produce nominally -689 MPa 100 ksi through-thickness compression on the loaded edge. The vanes were tested in cantilever loading conditions similar to the test methods used for the fan blades shown in Fig. 8. The fatigue strength of the LPB processed vanes even in the presence of a 0.5 mm 0.02 in. FOD approached the tensile yield strength of the material.

The high compression developed by LPB improves fatigue strength with and without FOD by retarding both crack initiation and growth. However, the benefit is most evident with surface damage present. The through-thickness compression superimposed upon the applied tensile stress shifts the mean stress toward or into compression, resulting in a higher allowed alternating stress. Fracture mechanics based fatigue life analysis using the AFGROW code confirms that for an edge crack growing in a thin plate through a zone of through-thickness compression, the endurance limit is nominally equal to the magnitude of compression present, and the depth of damage crack tolerated is approximately equal to the width of the zone of through-thickness compression measured from the edge.

Damage Tolerance Improvements in 17-4 PH Stainless Steel. Figure 11 shows the HCF performance of thick section

Fig. 10 Effect of LPB in mitigating HCF and FOD damage in a Ti-6-4 low pressure vane ” LPV …

Fig. 11 HCF performance of thick-section 17-4 PH stainless steel with 0.25 mm „0.010 in.… FOD for base line, shot peened and LPB surfaces

 

17-4 PH stainless steel. In this plot, the base-line data low-stress ground and buffed surface condition is compared with HCF data for shot peened and LPB conditions. The base-line fatigue strength is 930 MPa 135 ksi, only slightly lower than the 965 MPa 140 ksi strength of the shot peened condition. In contrast, LPB produced a fatigue strength in bending of 1240 MPa 180 ksi, exceeding the material’s tensile yield strength 1033 MPa 150 ksi due to the introduction of residual compression on the order of the yield strength.

The HCF performance without LPB dropped dramatically when 0.25 mm 0.01 in. deep by 0.76 mm 0.03 in. long FOD was introduced by EDM. As seen in Fig. 11, SP and the base-line fatigue strengths with FOD were only 276 MPa 40 ksi and 172 MPa 25 ksi, respectively. With the same FOD, the fatigue strength of LPB surface treated specimens was nominally 1033 MPa 150 ksi, comparable to the strength of the base-line material without FOD.

Mitigation of Corrosion Damage in Turbine Engine Alloys

Turbine engine components can be seriously affected by the presence of corrosion environments leading to pitting and significant debit in HCF lives. Salt spray corrosion pits are a common fatigue crack initiation site in ferritic stainless steels. Salt corrosion pitting can result from exposure to a marine atmosphere or steam turbine environments. Pitting depths, and the corresponding stress intensity factor, depend upon the time of exposure, temperature, and the service environment of the turbine engine. Salt pit corrosion typically reduces the endurance limit to nominally half of the uncorroded value. The effects of corrosion are often further exacerbated by the presence of FOD or erosion.

The effect of active corrosion during fatigue cycling on HCF behavior was monitored by exposing the thick section bend specimens to a corrosive medium during fatigue tests. A chemical-free absorbent pad soaked in an acidic salt solution 3.5 wt % NaCl, p H 3.5 was taped to the gauge section of the specimens and sealed to prevent evaporation with a thin plastic film. All other test conditions were as described earlier for studying thick-section HCF behavior. The effects of LPB on the active corrosion fatigue performance of Custom 450 stainless steel are presented in Fig. 12.

The low-stress ground base-line fatigue strength, tested in acid salt solution without FOD, was nominally 689 MPa 100 ksi. The base-line fatigue strength with 0.25 mm 0.01 in. FOD was only 69 MPa 10 ksi. In comparison, the LPB treated samples had fatigue strengths of over 1102 MPa 160 ksi in the corrosive

Fig. 12 Corrosion fatigue performance of Custom 450 stainless steel with FOD in acidic salt solution and FOD from 0.25 mm ” 0.010 in. … to 0.76 mm ” 0.030 in. …

 

environment alone, and 861 MPa 125 ksi, well above the baseline condition without FOD, with 0.25 mm 0.01 in. FOD. Although full S-N curves were not generated, when FOD depth was increased to 0.50 mm 0.02 in. and 0.76 mm 0.03 in., the further debit in HCF performance was minimal.

Mitigation of Fretting Fatigue Damage in Ti-6Al-4V

Fretting damage and the resulting HCF performance debit can reduce the HCF strength by 50% and limit the life of turbine engine fan and compressor dovetail joints. Fretting occurs where component surfaces are pressed into physical contact under loading conditions that produce small relative movement. Shallow shear stress cracks initiated at the edges of the fretting scars can grow in mode I to failure. Controlled fretting damage HCF tests were conducted on thick section Ti-6-4 to determine whether a deep layer of high residual compression produced by LPB could arrest the fretting induced shear cracking and prevent mode I propagation to failure, improving the fretting fatigue strength. Fretting damage was introduced into two sets of HCF samples both by pre-fretting the sample prior to fatigue testing to introduce prior damage, and by fretting during testing. Fretting damage was produced by pressing two Ti-6-4 alloy cylindrical rods with a 6.3 mm 0.25 in. diameter into the active gage surface of the fatigue specimen gage section using a bridge device to hold the rods. The rods were pressed into the fatigue specimen with a constant load of approximately 33.7 N 150 lbsi.e., 16.8 N per rod, producing a nominal contact stress of approximately 462 MPa 67 ksi. The fretting fixture was instrumented with strain gages and calibrated to record the normal load during testing. Figure 13 shows a photo of the fretting fixture positioned on a fatigue specimen.

The fretting fatigue results for thick section Ti-6-4 are shown in Fig. 14. Specimens were surface treated, exposed to simulated engine temperatures 375°C for 10 h and then subjected to fretting fatigue at room temperature. The fatigue strength for electropolished base-line Ti-6-4 tested at R 0.1 in four-point bending is nominally 482 MPa 70 ksi, which decreased drastically to about 172 MPa 25 ksi when subjected to fretting. Compressive residual stresses from shot peening provide significant benefit in restoring the fatigue strength to 413 MPa 60 ksi, nearly the base-line strength. In comparison, LPB produced nearly full restoration at 482 MPa 70 ksi. All but two LPB specimens tested at high stress levels 758 and 827 MPa 110 and 120 ksi failed outside of the LPB zone or sub-surface, with crack initiation from defects just below the compression zone, and not in the fretting scars.

Summary

The life of turbine engine and power systems is limited by fatigue, FOD, corrosion fatigue and fretting fatigue. Even small FOD, corrosion pits, or other surface damage can nucleate fatigue failures with catastrophic consequences. The cost of inspection and maintenance required to avoid fatigue failures is estimated in

Fig. 13 Photograph of the fretting fixture showing the top two fretting rods clamped onto the top surface of the thick section HCF specimen

Fig. 14 Ti-6Al-4V fretting fatigue data for shot peened and LPB surface treatments

 

the billions of dollars annually. Design or material changes generally provide only limited fatigue improvement at huge cost. Surface enhancement by LPB provides a thermally stable deep layer of compressive residual stress that can dramatically improve fatigue performance of turbine alloys without altering either alloy or design.

As summarized in this paper, the deep compression from LPB has been shown to resist thermal relaxation at turbine operating temperatures far better than conventional shot peening. The deep layer of compression has been shown to completely mitigate FOD up to 0.25 mm 0.01 in. deep in Ti-6-4, IN718 and 17-4 PH. Damage 1.27 mm 0.05 in. deep can be tolerated in Ti-6-4 blade edges. The corrosion fatigue strength of Carpenter 450 and fretting fatigue performance of Ti-6-4 can be substantially improved. Performance studies of other alloys are in process with comparable initial results.

LPB can be performed on conventional CNC machine tools in a conventional machine shop environment either in original manufacturing or during overhaul and repair. Residual stress distributions designed to cancel applied tension can be induced into the component surface to provide optimal fatigue performance at costs comparable to conventional machining. LPB offers the turbine designer a means, in addition to material selection and design, to improve turbine component performance and life at reduced operating costs.

Acknowledgment

Support for the development of the data presented here was provided under SBIR programs through NASA, Glenn Research Center, under the direction of Dr. Timothy Gabb; Wright Patterson AFB Materials Lab under the direction of Michael Shepard, the US Navy, NAVAIR, under the direction of Ravi Ravindranath, and with internal research support from Lambda Research. The financial support and technical guidance provided is gratefully acknowledged and much appreciated.

LPB Low plasticity burnishing SP Shot peening HCF High cycle fatigue EDM Electrical-discharge machining FOD Foreign object damage CW Cold work RS Residual stress XRD X-ray diffraction

References

Learn More About Our Technologies

Explore Lambda Technologies’ expertise in residual stress measurement and surface enhancement technologies.

Subscribe to our Mailing List

Thank you for subscribing!

Lambda Techs
Privacy Overview

This website uses cookies so that we can provide you with the best user experience possible. Cookie information is stored in your browser and performs functions such as recognising you when you return to our website and helping our team to understand which sections of the website you find most interesting and useful.